        滾珠絲桿斷裂分析報(bào)告

        關(guān)于這個(gè)問(wèn)題,深圳市漢工針對(duì)滾珠絲桿斷裂的原因給予解答:
        首先要弄清這個(gè)斷裂問(wèn)題,要了解很多細(xì)節(jié)問(wèn)題:
        1. 要對(duì)材質(zhì)進(jìn)行分析,
        2. 金相組織分析,
        3.表面硬度、芯部硬度檢查, 
        4. 斷口色澤、形貌特征分析。
         
        分析結(jié)果報(bào)告如下:
         
        1.金相分析
        (1)滲碳淬火硬化層組織:碳化物(Cm)3級(jí),馬氏體/殘奧(M/Ar)3級(jí);
        (2)心部組織:心部組織為板條馬氏體+鐵素體,芯部鐵素體(F)4級(jí);
        (3)芯部硬度:32~32.5HRC(在半圓橫切面上共檢測(cè)5個(gè)點(diǎn));
        (4)有效硬化層深度(CHD):0.95~1.03mm。
         
        2.材質(zhì)分析
        (1)光譜分析(%):0.221C,0.258Si,0.842Mn,0.027P,0.008S,1.107Cr,0.019Ni,0.004Mo,0.028Cu,0.039Al,0.062Ti,0.006V,0.008Co,<0.0001B,0.0006Ca,0.0002Mg,0.009As,
         
        0.003Pb,0.003Ce,<0.001La,0.004Bi;
        (2)化學(xué)分析(%):0.23C,0.26Si,0.92Mn,<0.035P,<0.035S,1.05Cr,0.078Ti。
         
        3.?dāng)嗫诜治?/span>
        從斷裂件斷口(經(jīng)酒精清洗后)的宏觀形貌上看,其斷口呈暗灰色,看不出任何晶界和晶面的痕跡。斷裂前產(chǎn)生了明顯的塑性滑移變形,這是一種比較典型的韌性斷口,亦有人稱其為纖維狀斷口,斷裂過(guò)程中吸收了較多的能量,一般是在高于材料屈服應(yīng)力條件下的高能斷裂。